SEM images of Mo2Ga2C MAX material
收藏数据链接:
官方服务:
资源简介:
In the dataset, are included SEM images of molybdenum gallium carbide MAX materials. The MAX materials were synthesised according to the procedure: 1) Gring of Mo2C powder with liquid gallium for 60 min in agate mortar at molar ration equal to Mo2C:Ga=1:10. 2)Transfer to the quartz ampule. 3) Evacuating and purging the ampule in order to remove oxygen. Closing the ampule under vacuum. 4) High-temperature annealing at 850 deg. C for 48 hours. The heating rate was maintained at 10 deg. C per minute. 5) Removing potentially formed oxides through leaching with 35% hydrochloric acid. 6) Drying under vacuum at 50 deg. C to dry mass.
创建时间:
2022-09-14